Hostname: page-component-7b7567c8c-m6dxt Total loading time: 0 Render date: 2026-11-19T00:20:47.287Z Has data issue: false hasContentIssue false

Additive manufacturing of nickel-based superalloy Inconel 718 by selective electron beam melting: Processing window and microstructure

Published online by Cambridge University Press:  11 August 2014

Harald Ernst Helmer*
Affiliation:
Zentralinstitut für Neue Materialien und Prozesstechnik (ZMP), University of Erlangen-Nuernberg, Fürth 90762, Germany
Carolin Körner
Affiliation:
Department of Materials Science, Chair of Metals Science and Technology, University of Erlangen-Nuernberg, Erlangen 91058, Germany
Robert Friedrich Singer
Affiliation:
Department of Materials Science, Chair of Metals Science and Technology, University of Erlangen-Nuernberg, Erlangen 91058, Germany
*
a) Address all correspondence to this author. e-mail: harald.e.helmer@fau.de

Abstract

Cube-shaped IN718 samples were produced by selective electron beam melting (SEBM) with varying beam power, deflection speed, and beam spot size. Process parameter windows were identified where fully dense samples are obtained with no surface unevenness. High deflection speeds were demonstrated to result in smaller demand of area energy. This result is explained by the reduced time for heat dissipation into the substrate during hatching. The grain structure was strongly affected by SEBM process parameters. Under certain conditions, epitaxial growth over many layers and well-developed columnar grain structures were obtained with a polycrystalline substrate plate. A more defocused beam led to a lower melt pool temperature and shallower melt pool geometry where maximum temperature gradients and solidification rates were more or less in parallel with the building direction and primary dendrite arm orientation. These conditions help to suppress grain nucleation ahead of the nucleation front as vigorous melt movement, fragmentation of dendrites, and tertiary arm growth are suppressed.

Information

Type
Articles
Copyright
Copyright © Materials Research Society 2014 
Figure 0

TABLE I.Nominal composition of gas atomized Inconel 718 powder and corresponding specification UNS N07718 (in wt%).

Figure 1

FIG. 1.Experimental setup for the IN718 test specimens. (a) Top surface view, (b) schematic illustrating hatching procedure. Specimens for microstructure evaluation were cut according to the plane shown in gray, i.e., with the plane of observation lying parallel to the BD and perpendicular to the hatching direction of the last layer.

Figure 2

FIG. 2.Examples of the top surface appearance of cube-shaped samples built in this investigation. (a) Sample with remaining porosity, (b) even top surface, (c) uneven top surface.

Figure 3

FIG. 3.Process parameter windows for IN718; suitable conditions resulting in dense samples with no top surface unevenness are indicated by black symbols. Process parameters varied are beam power and beam deflection speed. (a) Defocused beam (spot size = 500 µm) and (b) focused beam (spot size = 400 µm). Line distance is constant at 0.2 mm.

Figure 4

FIG. 4.Process parameter windows for IN718; suitable conditions resulting in dense samples with no top surface unevenness are indicated by black symbols and shaded area. Same data as in Fig. 3, but the beam energy per area EA [Eq. (1)] is being used to characterize processing conditions. (a) Defocused beam (spot size = 500 µm) and (b) focused beam (spot size = 400 µm). Line distance is constant at 0.2 mm. With higher deflection speeds, the area energy necessary to realize dense parts decreases. Higher deflection speeds lower the time available for heat loss by conduction. Focusing the beam lowers the area energy necessary even further. The more focused beam results in higher energy density, an effect which is not included in EA as defined by Eq. (1).

Figure 5

FIG. 5.The red open arrows depict the standard hatching pattern in SEBM: back and forth; the black arrow indicates the middle return line length sreturn, for which the thermal diffusion length is calculated [Eq. (3)].

Figure 6

FIG. 6.Processing window for IN718 in SEBM (focused beam, spot size = 400 µm), with area energy EA plotted as a function of thermal diffusion length lth. The area energy to obtain dense parts increases with increasing thermal diffusion length (decreasing scanning speeds) because of the increasing heat loss. At small lth values (high scanning speeds), the theoretical minimum area energy EA is approached (dotted line). The theoretical minimum area energy corresponds to the energy necessary to heat and to melt a 150 µm layer of IN718 material.

Figure 7

FIG. 7.Optical micrograph showing columnar grain structure in a longitudinal section parallel to the BD. (Beam parameters: defocused beam, spot size of 500 µm, v = 200 mm s−1, P = 200 W.) A consolidated layer thickness of 50 µm was used.

Figure 8

FIG. 8.Mean grain width in dependence of the build height. The grain width is increasing with the build height due to a grain selection process. (Beam parameters: defocused beam, spot size of 500 µm, v = 200 mm s−1, P = 200 W.)

Figure 9

FIG. 9.Optical micrograph showing a view of the last fabricated layer next to the top surface of the sample. Specimen was cut perpendicular to the last hatching direction, i.e., the beam was moving as shown in Fig. 10(b). (Beam parameters: defocused beam, spot size of 500 µm in (a) and focused beam, spot size of 400 µm in (b); v = 200 mm s−1 and P = 200 W same for both.) In (a), the insert in the top corner shows the dendrite structure in a higher magnification. In (b), the melt pool dimensions are outlined for better visualization. The preferred crystallographic orientation is shown on the right.

Figure 10

FIG. 10.Schematic illustrating melt pool geometry. Cross-sectional view parallel to the direction of beam motion in (a) and perpendicular to the direction of beam motion in (b). The liquidus isotherm normal is equivalent to the direction of the main temperature gradient G and solidification rate vS. The melt pool shape for the defocused beam is shallower than that for the focused beam, i.e., the temperature gradient driving solidification deviates less from the BD and primary dendrite arm orientation.

Figure 11

FIG. 11.Dendrite structure and melt pool geometry as in Fig. 9, but larger section size extending over several layers. (a) Optical micrograph defocused beam. (b) Optical micrograph focused beam. (c) Schematic explaining melt pool geometry and hatching strategy. The hatching direction is altered by 90° after each layer as described in Fig. 1. Specimens were cut perpendicular to the BD. (Beam parameters: defocused beam with a spot size of 500 µm; focused beam with a spot size of 400 µm; v = 200 mm s−1, and P = 200 W.) Beam focus influences the melt pool shape leading to a shallower geometry with less curvature of the interface for a defocused beam.

Figure 12

FIG. 12.EBSD orientation maps and according to the pole figures of SEBM samples fabricated with a defocused beam in (a–b) and a focused beam in (c–d). (Beam parameters: v = 200 mm s−1 and P = 200 W.) Specimens were cut parallel to the BD (= Y in the sample coordinate system on the left). In (a) and (c), IPF-maps are shown with colored crystallographic orientations relative to the sample axis X. Stray grains can be observed for the focused beam in (c) indicating nucleation ahead of the solidification front. This results in a texture with less strongly aligned grains. For the defocused beam, grains are well aligned to the BD (sample axis Y), see pole figures (Z–X plane) in (b) and (d). The crystal orientation-color relation map is shown on the left.

Figure 13

FIG. 13.Mean grain width (mean intercept) of SEBM samples of the process window in Fig. 4 (beam spot size of 500 µm and 400 µm), measured in a plane parallel to the BD at a build height of 9 mm [corresponding power values of the measured samples can be found in Figs. 3(a) and 3(b)]. With the focused beam, a smaller grain width is observed indicating more nucleation ahead of the solidification front.