Hostname: page-component-7b7567c8c-qz9hd Total loading time: 0 Render date: 2026-11-30T19:46:46.326Z Has data issue: false hasContentIssue false

Time-dependent mechanical properties of rat femoral cortical bone by nanoindentation: An age-related study

Published online by Cambridge University Press:  04 June 2014

Sebastián Jaramillo Isaza*
Affiliation:
Department of Biological Engineering, Laboratoire de Biomécanique et Bioingénierie, UMR CNRS-UTC 7338, Université de Technologie de Compiègne, Compiègne Cedex 60205, France
Pierre-Emmanuel Mazeran
Affiliation:
Department of Mechanical Systems, Laboratoire Roberval Unité de Recherche en Mécanique, UMR CRNS-UTC 7337, Université de Technologie de Compiègne, Compiègne Cedex 60205, France
Karim El Kirat
Affiliation:
Department of Biological Engineering, Laboratoire de Biomécanique et Bioingénierie, UMR CNRS-UTC 7338, Université de Technologie de Compiègne, Compiègne Cedex 60205, France
Marie-Christine Ho Ba Tho*
Affiliation:
Department of Biological Engineering, Laboratoire de Biomécanique et Bioingénierie, UMR CNRS-UTC 7338, Université de Technologie de Compiègne, Compiègne Cedex 60205, France
*
a) Address all correspondence to this author. e-mail: marie-christine.hobatho@utc.fr

Abstract

The aim of this study is to assess the time-dependent mechanical properties of rat femoral cortical bone in a lifespan model from growth to senescence. New nanoindentation protocol was performed to assess the time-dependent mechanical behavior. The experimental data were fitted with an elastic–viscoelastic–plastic–viscoplastic mechanical model allowing the calculus of the mechanical properties. Variation of mechanical response of bone as a function of the strain rate and age were highlighted. The most representative variations of the mechanical properties with age were found to be statistically significant (P < 0.001) from 1 to 4 months for elastic properties, from 1 to 9 months for viscoelastic properties and during all lifespan for plastic and viscoplastic properties, highlighting different maturation ages for elastic, viscoelastic, plastic and viscoplastic behaviors. These results suggest that different physical–chemical and structural processes occur at different ages reflecting bone modeling and remodeling activities in the rat's whole lifespan.

Information

Type
Articles
Copyright
Copyright © Materials Research Society 2014 
Figure 0

FIG. 1.Material mechanical model used to describe the mechanical behavior of the rat femoral cortical bone. This model is composed of an elastic modulus, two viscoelasticities with different time-constants, a plasticity and a viscoplasticity.

Figure 1

FIG. 2.Indentation depth ht (red curve) and sum of the displacement of the mechanical model elements dp (black dashed line) versus time during the nanoindentation experiment. An excellent agreement was found between experimental data and the fit proposed by the mechanical model.

Figure 2

TABLE I.Equations used to assess the mechanical properties from the nanoindentation model. The values of the displacement of the different elements are taken at the beginning of the unloading curve, point of the curve from which the contact area is computed.

Figure 3

TABLE II.Values of the mechanical properties computed from the nanoindentation experiments in the longitudinal direction of the rat femoral cortical bone.

Figure 4

FIG. 3.Variation of elastic modulus Eelast of the rat femoral cortical bone with age. Symbol “•” represents the mean value. (Significant differences from the DSCF test *P< 0.001 and **P < 0.05).

Figure 5

FIG. 4.Variation of viscoelastic moduli of the rat femoral cortical bone with age: Elastic components ((a) and (c)) and the viscous component ((b) and (d)). Symbol “•” represents the mean value. (Significant differences from the DSCF test *P< 0.001 and **P < 0.05).

Figure 6

FIG. 5.Variation of hardness (a) and viscoplasticity (b) of the rat femoral cortical bone with age. Symbol “•” represents the mean value. (Significant differences from the DSCF test *P< 0.001 and **P < 0.05).

Figure 7

FIG. 6.Apparent elastic modulus as a function of age and strain rate: From top to bottom strain rate $\dot \varepsilon$= ∞ 0.05 s−1 and 0. DSCF test shows that variation is statistically significant from 1 to 4 months old (P < 0.001).

Figure 8

TABLE III.Values of the apparent elastic modulus of the rat femoral cortical bone as a function of the strain rate and the age of the samples.

Figure 9

TABLE IV.Maturation age of different mechanical properties for male rats RJHan:WI Wistar computed at the 95% of the estimated asymptote.

Figure 10

TABLE V.Mean values reported using nanoindentation for the reduced modulus and hardness in different animal models.