Hostname: page-component-7b7567c8c-wxvwp Total loading time: 0 Render date: 2026-11-17T11:34:53.355Z Has data issue: false hasContentIssue false

Zirconium Mediated Hydrogen Outdiffusion From p-GaN

Published online by Cambridge University Press:  13 June 2014

E. Kaminska
Affiliation:
Institute of Electron Technology, Al.Lotnikow 46, Warsaw, Poland. eliana@ite.waw.pl.
A. Piotrowska
Affiliation:
Institute of Electron Technology, Al.Lotnikow 46, Warsaw, Poland. eliana@ite.waw.pl.
A. Barcz
Affiliation:
Institute of Electron Technology, Al.Lotnikow 46, Warsaw, Poland. eliana@ite.waw.pl.Institute of Physics PAS, Warsaw, Poland
J. Jasinski
Affiliation:
Institute of Experimental Physics, Warsaw University, Warsaw, Poland
M. Zielinski
Affiliation:
Institute of Physics PAS, Warsaw, Poland
K. Golaszewska
Affiliation:
Institute of Electron Technology, Al.Lotnikow 46, Warsaw, Poland. eliana@ite.waw.pl.
R.F. Davis
Affiliation:
Department of Material Science and Eng., NCSU, Raleigh, NC 27695-7907, USA
E. Goldys
Affiliation:
SMPCE, Macquarie University, Sydney NSW, Australia
K. Tomsia
Affiliation:
SMPCE, Macquarie University, Sydney NSW, Australia

Abstract

We have shown that Zr-based metallization can effectively remove hydrogen from the p-type GaN subsurface, which eventually leads to the formation of an ohmic contact. As the release of hydrogen starts at ∼900°C, the thermal stability of the contact system is of particular importance. The remarkable thermal behavior of the ZrN/ZrB2 metallization is associated to the microstructure of each individual Zr-based compound, as well as to the interfacial crystalline accommodation.

Information

Type
Research Article
Copyright
Copyright © 1996 Materials Research Society
Figure 0

Figure 1.XTEM micrographs of GaN/ZrN/ZrB2 contact: a) as-deposited, b) annealed at 800°C, 5 min., c) annealed at 1100°C, 30 s.

Figure 1

Figure 2.SIMS profiles for GaN/ZrN/ZrB2 contact: a) as-deposited, b) annealed at 800°C, 5 min., c) annealed at 1100°C, 30 s.

Figure 2

Figure 3.HREM images of GaN/ZrN interface after annealing at: a) 800°C, 5 min., b) 1100°C, 30 s.

Figure 3

Table I.Relative H- yields with respect to Zr- in ZrN and ZrB2 films after annealing.

Figure 4

Figure 4.Magnesium and hydrogen depth profiles in p-GaN annealed under ZrN/ZrB2: a) as-deposited and annealed at 800°C, 5 min., b) as-deposited and annealed at 1100°C, 30 s.