Temperature-dependent nanoindentation response of materials

Published online by Cambridge University Press:  20 February 2018

Saeed Zare Chavoshi*
Affiliation:
Department of Mechanical Engineering, Imperial College London, London SW7 2AZ, UK
Shuozhi Xu
Affiliation:
California NanoSystems Institute, University of California, Santa Barbara, Santa Barbara, CA 93106-6105, USA
*
Address all correspondence to Saeed Zare Chavoshi at s.zare@imperial.ac.uk

Abstract

It is of the uttermost interest to understand the mechanical performance and deformation mechanisms contributing to small-scale plasticity of materials in micro/nanoelectromechanical systems at their service temperatures, which are usually above room temperature. In recent years, high-temperature nanoindentation experiments have emerged as a reliable approach to characterize the deformation behavior of materials at the nano and submicron scale. In this review, we highlight the role of the temperature in nanoindentation response of a wide variety of materials, with a particular focus on the thermally-activated deformation mechanisms in crystalline and non-crystalline materials under the indenter, e.g., dislocation processes, shear transformation zone, and phase transformations. A brief survey of the temperature-dependent nanoindentation elastic modulus, hardness, and creep behavior of materials is also provided. We also discuss experimental methods for correctly measuring the mechanical properties of materials at high temperatures.

Information

Type
Prospective Articles
Copyright
Copyright © Materials Research Society 2018 
Figure 0

Figure 1.Temperature-dependent phenomena in materials during high-temperature nanoindentation.

Figure 1

Figure 2.Dark-field TEM of the indentation imprint on Mg17Al12. More homogeneous dislocation distribution exhibiting a curved shape with some dissociation is seen at the high temperature. Adopted with permission from Ref.[19] (Elsevier, 2016).

Figure 2

Figure 3.(a) P-h curves from the nanoindentation of Ta at a loading rate of 1000 µN/s at different temperatures, (b) Elastic-plastic and elastic fit; the dashed curve is from experiments at 23 °C. Friction coefficient decreases with temperature. Adopted with permission from Ref.[22] (Taylor & Francis, 2010).

Figure 3

Figure 4.(a) P-h curves from the nanoindentation of Pt (100) at different temperatures, (b) cumulative fraction of pop-in events. Displacement bursts increase with temperature. Adopted with permission from Ref.[28] (American Institute of Physics, 2004).

Figure 4

Figure 5.Topographic images of two indentations in Pt-based metallic glass at 176 and 250 °C after unloading, illustrating relative stability and substantial shape recovery, respectively. h in the legend indicates the surface roughness. Adopted with permission from Ref.[42] (Elsevier, 2009).

Figure 5

Figure 6.(a) In-situ scanning electron microscopy (SEM) pile-up deformation of a Zr-based BMG at 25 °C and 200 °C, (b) P-h curves for indentations loaded at 1 mN/s at different temperatures, (c) Hardness and reduced modulus as a function of temperature. Adopted with permission from Ref.[45] (Elsevier, 2011).

Figure 6

Figure 7.P-h curves of pristine Si (c-Si), relaxed and unrelaxed a-Si at (a) 25 °C and (b) 200 °C. Unusual “bowing” behavior of pristine Si at 200 °C is observable. Relaxed a-Si shows a “pop-out” event. Adopted with permission from Ref.[52] (Cambridge University Press, 2012).

Figure 7

Figure 8.Deformation of relaxed a-Si at different temperatures. Adopted with permission from Ref.[54] (American Institute of Physics, 2014).

Figure 8

Figure 9.(a) and (b) Bright-field and (c) and (d) Dark-field XTEM images along with the SAD patterns of Berkovich indents indented on Si. Diffraction spots from bc8/r8 are pointed to by red arrows. The yellow arrows in (c) and (d) represent twinning and in their corresponding SAD patterns represent streaking and spot splitting due to twinning, respectively. For clarity, the red lines in (a), (b), and (c) illustrate the boundary between phase transformed and untransformed volumes under the indenter. Adopted with permission from Ref.[57] (American Institute of Physics, 2015).

Figure 9

Figure 10.Schematic of the temperature dependence of the deformation mechanisms of diamond cubic Si under a nanoscale Berkovich indenter. Adopted with permission from Ref.[57] (American Institute of Physics, 2015).

Figure 10

Figure 11.TEM bright-field image demonstrating (a) Phase transformation in Ge, marked ‘t’, at room temperature, (b) Hexagonal crystal structure (‘cr’) and twinning (‘tw’) at 400 °C. Adopted with permission from Ref.[58] (Elsevier, 2007).

Figure 11

Figure 12.Percentage of (a) hardness (b) Young's modulus reduction as a function of temperature. The percentage values are calculated with respect to their values at room temperature. For further information, see Table 1.

Figure 12

Figure 13.Indentation hardness of high-purity Cr as a function of temperature and strain-rate. Adopted with permission from Ref.[32] (Elsevier, 2017).

Figure 13

Table I.Overview of nanoindentation mechanical responses of different materials at high temperatures.