Hostname: page-component-7b7567c8c-wxvwp Total loading time: 0 Render date: 2026-11-17T21:27:41.486Z Has data issue: false hasContentIssue false

Metal/GaN contacts studied by electron spectroscopies

Published online by Cambridge University Press:  13 June 2014

J. Dumont
Affiliation:
Facultés Universitaires Notre-Dame de la Paix, Laboratoire Interdisciplinaire de Spectroscopie Electronique, Namur, Belgium
R. Caudano
Affiliation:
Facultés Universitaires Notre-Dame de la Paix, Laboratoire Interdisciplinaire de Spectroscopie Electronique, Namur, Belgium
R. Sporken
Affiliation:
Facultés Universitaires Notre-Dame de la Paix, Laboratoire Interdisciplinaire de Spectroscopie Electronique, Namur, Belgium
E. Monroy
Affiliation:
Universidad Politecnica de Madrid, E.S.T.I., Ciudad Universitaria, Madrid, Spain
E. Muñoz
Affiliation:
Universidad Politecnica de Madrid, E.S.T.I., Ciudad Universitaria, Madrid, Spain
B. Beaumont
Affiliation:
Centre de Recherche sur l’Hetero-Epitaxie et ses Applications, CRHEA-CNRS, Valbonne, France
P. Gibart
Affiliation:
Centre de Recherche sur l’Hetero-Epitaxie et ses Applications, CRHEA-CNRS, Valbonne, France

Abstract

Au/GaN and Cu/GaN Schottky contacts have been studied using X-ray Photoelectron Spectroscopy (XPS) and Auger Electron Spectroscopy (AES). Clean and stoechiometric GaN samples were obtained using in situ hydrogen plasma treatment and Ga deposition. The growth of Cu and Au follows Stranski-Krastanov and Frank van der Merwe modes respectively. The interfaces are sharp and non-reactive. Schottky barriers of 1.15eV for Au/GaN and 0.85eV for Cu/GaN were measured using XPS.

Information

Type
Research Article
Copyright
Copyright © 1996 Materials Research Society
Figure 0

Figure. 1Left: Auger spectra of GaN cleaned following different procedures: (a) untreated; (b) cycles of boiling HNO3 and deionized water; (c) same as (b), followed by H* exposure at 600°C;(d) same as (b) followed by Ga deposition and desorption at 950°C. Right: XPS spectra of GaN surfaces: (a) untreated; (b) cycles of H* exposure followed by Ga deposition + desorption.

Figure 1

Figure. 2:Ga2p3/2 and Cu2p3/2 XPS spectra during formation of the Cu/GaN interface.

Figure 2

Figure. 3.Experimental and calculated XPS intensities during the growth of Cu on GaN. Left: calculated intensities for layer by layer growth mode. Right: calculated intensities for modified Stranski-Krastanov growth mode .

Figure 3

Table I:photoelectron mean free paths. 1st column: λ calculated using the Seah and Dench formula. [8] Other columns: values obtained from the XPS intensities. ρ2D = density of the 2D layer; N2D = number of atoms per unit area in the 2D layer.

Figure 4

Figure. 4Left: position of the Fermi level with respect to the valence band maximum, as a function of Cu coverage. Right: Cu L3M45M45 Auger features; evolution with copper coverage.