Hostname: page-component-7b7567c8c-z4zkx Total loading time: 0 Render date: 2026-11-17T22:49:22.414Z Has data issue: false hasContentIssue false

Influence of Si-Doping on Carrier Localization of Mocvd-grown InGaN/GaN Multiple Quantum Wells

Published online by Cambridge University Press:  13 June 2014

Yong-Hoon Cho
Affiliation:
Center for Laser and Photonics Research and Department of Physics Oklahoma State University, Stillwater, OK 74078
T. J. Schmidt
Affiliation:
Center for Laser and Photonics Research and Department of Physics Oklahoma State University, Stillwater, OK 74078
S. Bidnyk
Affiliation:
Center for Laser and Photonics Research and Department of Physics Oklahoma State University, Stillwater, OK 74078
J. J. Song
Affiliation:
Center for Laser and Photonics Research and Department of Physics Oklahoma State University, Stillwater, OK 74078
S. Keller
Affiliation:
Electrical and Computer Engineering and Materials Departments University of California, Santa Barbara, CA 93106
U. K. Mishra
Affiliation:
Electrical and Computer Engineering and Materials Departments University of California, Santa Barbara, CA 93106
S. P. DenBaars
Affiliation:
Electrical and Computer Engineering and Materials Departments University of California, Santa Barbara, CA 93106

Abstract

We have systematically studied the influence of Si doping on the optical characteristics of InGaN/GaN multiple quantum wells (MQWs) using photoluminescence (PL), PL excitation (PLE), and time-resolved PL spectroscopy combined with studies of optically pumped stimulated emission and structural properties from these materials. The MQWs were grown on 1.8-μm-thick GaN layers on c-plane sapphire films by metalorganic chemical vapor deposition. The structures consisted of 12 MQWs with 3-nm-thick InGaN wells, 4.5-nm-thick GaN barriers, and a 0.1-μm-thick Al0.07Ga0.93N capping layer. The Si doping level in the GaN barriers was varied from 1 × 1017 to 3 × 1019 cm−3. PL and PLE measurements show a decrease in the Stokes shift with increasing Si doping concentration. The 10 K radiative recombination lifetime was observed to decrease with increasing Si doping concentration (n), from ∼ 30 ns (for n < 1 × 1017 cm−3) to ∼ 4 ns (for n = 3 × 1019 cm−3). To elucidate whether non-radiative recombination processes affect the measured lifetime, the temperature-dependence of the measured lifetime was investigated. The reduced Stokes shift, the decrease in radiative recombination lifetime, and the increase in structural and interface quality with increasing Si doping indicate that the incorporation of Si in the GaN barriers results in a decrease in carrier localization at potential fluctuations in the InGaN active regions and the interfaces.

Information

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society
Figure 0

Figure 1.10 K PL (solid lines), PLE (dashed lines), and TRPL data (open circles) of 12-period InGaN/GaN MQWs with Si doping concentrations ranging from < 1 × 1017 to 3 × 1019 cm−3 in the GaN barriers. The Stokes shift between the PL emission peak and the absorption band-edge observed from PLE spectra decreases significantly as the Si doping concentration increases. Luminescence decay times measured by TRPL are shown as a function of emission energy. With increasing Si doping concentration, the 10 K lifetimes decrease from ∼ 30 ns (for n < 1 × 1017 cm−3) to ∼ 4 ns (for n = 3 × 1019 cm−3).

Figure 1

Figure 2.Temperature dependence of decay times monitored above (up triangles), below (down triangles), and at (circles) the emission peak for the InGaN/GaN MQWs with n < 1 × 1017 cm−3 (open symbols) and n = 3 × 1019 cm−3 (closed symbols) in the GaN barriers. The characteristic crossover temperature, Tc, (which is determined by the radiative and non-radiative recombination rates) gradually increases as n increases: Tc ∼ 70 K for n < 1 × 1017 cm−3, Tc ∼ 100 K for n = 2 × 1018 cm−3 (not shown), and Tc ∼ 140 K for n = 3 × 1019 cm−3.

Figure 2

Figure 3.2 μm × 2 μm AFM images of three 7-nm-thick GaN films with different disilane flow rates during growth. The root-mean-square surface roughness estimated from AFM images was 0.49, 0.42, and 0.22 nm for GaN epilayers with the disilane flow rate of (a) 0, (b) 0.2, and (c) 2 nmol/min, respectively. A higher quality GaN surface morphology and a larger average terrace length were achieved by increasing Si incorporation.