Hostname: page-component-7b7567c8c-wxvwp Total loading time: 0 Render date: 2026-11-18T04:25:21.287Z Has data issue: false hasContentIssue false

GaN Homoepitaxy for Device Applications

Published online by Cambridge University Press:  13 June 2014

M. Kamp
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
C. Kirchner
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
V. Schwegler
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
A. Pelzmann
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
K.J. Ebeling
Affiliation:
Dept. of Optoelectronics, University of Ulm, 89069 Ulm, GERMANY, Tel.: +49-731-5026050, Fax: +49-731-5026049, e-mail: markus.kamp@e-technik.uni-ulm.de
M. Leszczynski
Affiliation:
High Pressure Research Center, Warsaw, POLAND
I. Grzegory
Affiliation:
High Pressure Research Center, Warsaw, POLAND
T. Suski
Affiliation:
High Pressure Research Center, Warsaw, POLAND
S. Porowski
Affiliation:
High Pressure Research Center, Warsaw, POLAND

Abstract

Epitaxial growth on GaN single bulk crystals sets new standards in GaN material quality. The outstanding properties provide new insights into fundamental material parameters (e.g. lattice constants, exciton binding energies, etc.) being not accessible by heteroepitaxial growth on sapphire or SiC. With MOVPE and MBE we realized unstrained GaN layers with dislocation densities about six orders of magnitude lower than in heteroepitaxy. Those layers revealed an exceptional optical quality as determined by a reduction of the photoluminescence linewidth from 5 to 0.1 meV and a reduced XRD rocking curve width from 400 to 20 arcsec.

Only recently, progress in surface preparation allowed morphologies of the layers suitable for device applications. We report on InGaN/GaN MQW structures as well as the first GaN pn- and InGaN/GaN double heterostructure LEDs on GaN single bulk crystals. Those LEDs are twice as bright as their counterparts grown on sapphire. In addition they reveal an improved high power characteristics, which is attributed to an enhanced crystal quality and an increased p-doping. Time resolved electroluminescence measurements proof that band/band recombination is the dominant emission mechanism for the InGaN/GaN LEDs.

Information

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society
Figure 0

Fig 1.:Photoluminescence of epitaxial GaN layers (MBE) on (000−1)- and (0001)-oriented GaN substrates. Linewidth is as low as 0.5 meV for the (0001)-orientation.

Figure 1

Fig 2.:SEM image (2a), corresponding cathodoluminescence (CL) intensities (2b) and local CL spectra (2c) obtained from an epitaxial GaN layer grown on partially CAIBE treated (0001)-oriented GaN substrates. CL by F. Bertram, T. Riemann, and J. Christen (Univ. Magdeburg).

Figure 2

Fig. 3:SEM micrograph of the surface of a homoepitaxial GaN pn-junction LED with evaporated Ni/Au metal contacts, without (3a) and with (3b) CAIBE treatment prior to growth (different areas of the same sample).

Figure 3

Fig. 4:High resolution photoluminescence (log. scale) and reflectance (lin. scale) of a 2 µm epitaxial GaN layer grown on CAIBE treated (0001)-oriented GaN substrates. Measurements by K. Kornitzer, K. Thonke, and R. Sauer (Univ. Ulm, Dept. of Semiconductor Physics).

Figure 4

Fig. 5:Room temperature photoluminescence of approx. 50 nm InGaN layers grown on GaN- and sapphire-substrates, respectively.

Figure 5

Fig. 6:Photoluminescence of InGaN/GaN (3nm/3nm) multiple quantum well structures grown on GaN- and sapphire-substrates, respectively (20 K).

Figure 6

Fig. 7:Electroluminescence (EL) of a GaN homojunction pn-LED grown on GaN substrate. Emission spectra at various current densities. At a given current density, the homoepitaxial devices are twice as bright as comparable LEDs grown on sapphire (dashed line).

Figure 7

Fig. 8:Electroluminescence (EL) of a InGaN/GaN DH-LED grown on GaN substrate. Excellent EL is achieved at low current densities, revealing a low density of non-radiative defects.

Figure 8

Fig. 9:Time resolved electroluminescence (EL) of a InGaN/GaN DH-LED grown on GaN substrate. Depicted is the EL after short-pulse-excitation at 50 V for 10 ns (pulse being also depicted). Exponential decay time is as short as 1 ns indicating band/band recombination. The pulse-signal delay of 35 ns is caused by the experimental setup.

Figure 9

Fig. 10:Current/voltage characteristics of a GaN InGaN/GaN DH-LED. The curve reveals a good breakdown behavior and turn-on-voltage but still a rather high series resistance. The later is probably originated by contributions from the silver glue (n-contact metal) and the 200 − 300 µm thick n-layer (i.e. mostly the substrate).