Hostname: page-component-7b7567c8c-tnkh4 Total loading time: 0 Render date: 2026-11-18T19:26:05.937Z Has data issue: false hasContentIssue false

Group-III Nitride ETCH Selectivity IN BCl /Cl ICP Plasmas

Published online by Cambridge University Press:  13 June 2014

R. J. Shul
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-0603, rjshul@sandia.gov
L. Zhang
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-0603, rjshul@sandia.gov
C. G. Willison
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-0603, rjshul@sandia.gov
J. Han
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-0603, rjshul@sandia.gov
S. J. Pearton
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-0603, rjshul@sandia.gov
J. Hong
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-0603, rjshul@sandia.gov
C. R. Abernathy
Affiliation:
Sandia National Laboratories, Albuquerque, NM 87185-0603, rjshul@sandia.gov
Lester
Affiliation:
University of New Mexico, Electrical Engineering, Albuquerque, NM

Abstract

Patterning the group-III nitrides has been challenging due to their strong bond energies and relatively inert chemical nature as compared to other compound semiconductors. Plasma etch processes have been used almost exclusively to pattern these films. The use of high-density plasma etch systems, including inductively coupled plasmas (ICP), has resulted in relatively high etch rates (often greater than 1.0 µm/min) with anisotropic profiles and smooth etch morphologies. However, the etch mechanism is often dominated by high ion bombardment energies which can minimize etch selectivity. The use of an ICP-generated BCl3 /Cl2 plasma has yielded a highly versatile GaN etch process with rates ranging from 100 to 8000 Å/min making this plasma chemistry a prime candidate for optimization of etch selectivity. In this study, we will report ICP etch rates and selectivities for GaN, AlN, and InN as a function of BCl3/Cl2 flow ratios, cathode rf-power, and ICP-source power. GaN:InN and GaN:AlN etch selectivities were typically less than 7:1 and showed the strongest dependence on flow ratio. This trend may be attributed to faster GaN etch rates observed at higher concentrations of atomic Cl which was monitored using optical emission spectroscopy (OES).

Information

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society
Figure 0

Figure 1.OES of ICP generated BCl3 /Cl2

Figure 1

Figure 2.GaN, InN, and AlN etch rates as a function of %Cl2 in a BCl3 /Cl2 /Ar ICP plasma. Plasma conditions were: 2 mTorr pressure, 500 W ICP-source power, 125 W cathode rf-power, and 25°C cathode temperature.

Figure 2

Figure 3.OES showing the increase in Cl+ and Cl0 emission normalized to Ar as a function of %Cl2 concentration.

Figure 3

Figure 4.GaN:AlN and GaN:InN etch selectivities as a function of %Cl2 in a BCl3 /Cl2 /Ar ICP plasma. Plasma conditions were: 2 mTorr pressure, ICP-source power 500 W, 125 W cathode rf-power, and 25°C cathode temperature.

Figure 4

Figure 5.GaN, InN, and AlN etch rates as a function of cathode rf-power in a BCl3 /Cl2 /Ar ICP plasma. Plasma conditions were: 2 mTorr pressure, ICP-source power 500 W, 32 sccm Cl2, 8 sccm BCl3, and 25°C cathode temperature.

Figure 5

Figure 6.GaN:AlN and GaN:InN etch selectivities as a function of cathode rf-power in a BCl3 /Cl2 /Ar ICP plasma. Plasma conditions were: 2 mTorr pressure, ICP-source power 500 W, 32 sccm Cl2 , 8 sccm BCl3 , and 25°C cathode temperature.

Figure 6

Figure 7.GaN, InN, and AlN etch rates as a function of ICP source power in a BCl3 /Cl2 /Ar plasma. Plasma conditions were: 2 mTorr pressure, 125 W cathode rf-power with corresponding dc-bias ranging from −160 to −300 V, 32 sccm Cl2 , 8 sccm BCl3 , and 25°C cathode temperature.

Figure 7

Figure 8.GaN:AlN and GaN:InN etch selectivities as a function of ICP source power in a BCl3 /Cl2 /Ar plasma. Plasma conditions were: 2 mTorr pressure, 125 W cathode rf-power with corresponding dc-bias ranging from −160 to −300 V, 32 sccm Cl2 ,cathode temperature.

Figure 8

Figure 9.GaN, AlN, and normalized InN rms roughness as a function of %Cl2 ICP etch conditions were 32 sccm Cl2 , 8 sccm BCl3, 5 sccm BCl3 , 5 sccm Ar, 500 W ICP source power, and 2 mTorr pressure.

Figure 9

Figure 10.SEM micrographs for GaN etched at a) −50, b) −150, and c) −300 V dc-bias. ICP etch conditions were 32 sccm Cl2 , 8 sccm BCl3 , 5 sccm Ar, 500 W ICP power, and 2 mTorr pressure.