Hostname: page-component-7b7567c8c-2n9c9 Total loading time: 0 Render date: 2026-11-17T20:19:34.535Z Has data issue: false hasContentIssue false

Focused Ion Beam Micromachining of GaN Photonic Devices

Published online by Cambridge University Press:  13 June 2014

Abstract

Ga+ and Au+ focused ion beams (FIB) are used to micromachine GaN films. The GaN micromachining has been studied at energies from 30-90 keV, incident angle from 0-30°, and number of repetitive scans from 10 to 50 scans. Trenches milled in GaN have vertical and smooth side-walls and very smooth bottoms. The micromachining rate was found to be fairly independent of ion dose, ranging from 0.4 to 0.6 µm3 /nC for Ga+ and 1 to 2 µm3 /nC for Au+. This translates into an effective yield of of 6-7 atoms/ion for Ga+ and 21-26 atoms/ion for Au+. This represents the highest direct FIB removal yield reported to date. We have also investigated the micromachining of GaN substrate material: c-face sapphire. Using FIB Ga+, sapphire has an effective yield of ∼2-2.5 atoms/ion, or approximately 1/3 of the GaN sputtering yield. For the materials investigated, we found the sputtering yield to be inversely proportional to the strength of the material chemical bond. We also describe the application of the FIB μmachining technique to the fabrication of small period Distributed Bragg Reflector (DBR) mirrors for a short cavity GaN laser structure.

Information

Type
Research Article
Copyright
Copyright © 1999 Materials Research Society
Figure 0

Fig. 1The Ga+ FIB micromachined pattern: (a) SEM photograph of GaN pattern micromachined using 90kV Au+ FIB with a dose of 1×1018cm−2, at normal incidence, and 10 scans; (b) schematic diagram of serpentine scan.

Figure 1

Fig. 2Ga+ milling rate of GaN versus angle of incidence for different energies in 10 FIB scans. (total dose: 1 ×1018cm−2)

Figure 2

Fig. 3Ga+ milling rate of GaN versus angle of incidence for different scan conditions at 50 keV. (total dose: 1 ×1018cm−2)

Figure 3

Fig. 4Au+ milling rate of GaN versus ion energy for different scan conditions in the normal incidence. (total dose: 1×1018cm−2)

Figure 4

Fig. 5Comparison of Ga+ and Au+ milling rate of GaN and sapphire as a function of ion energy (total dose: 1×1018cm−2, normal incidence, 10 scans)

Figure 5

Fig. 6The SEM photographs of the GaN laser with DBR gratings by FIB micromachining: (a) the overview of laser structure, cavity length is 120 μm; (b) the 5th order grating structure, the period is 675 nm and spacing is 200 nm..